An epoxy floor that goes wrong usually tells you why. Where it lifts, how the blisters feel, whether the marks are on the surface or through it: each points back to a cause, and the cause decides the fix. This page goes through every common fault one at a time, using what the UK resin makers put on their own data sheets, so you can work out what happened to your floor and what it takes to put right.
Symptom, cause and fix (scan this first)
| What you see | Usual cause | Fix |
|---|---|---|
| Coating peeling or lifting in sheets | Laitance left on, power-floated or sealed concrete, old paint underneath, oil, cold or damp during the cure | Grind off everything loose, back to sound concrete, and start again |
| Swollen pockets, sometimes with liquid in them | Damp pushed up through the slab after the floor cured (osmotic blistering) | Fix the moisture first: damp-tolerant primer or a surface membrane, then recoat |
| Tiny holes, craters or bubbles | Air rising out of porous concrete, no primer, primer left too long, over-mixing | Sand the area and patch with the topcoat; prime properly next time |
| White, matt or greasy film | Blooming (amine blush): cold, humid air or condensation while it cured | Clean it off and key the surface before any further coat |
| Tyre marks or patches pulled off where the car sits | Hot tyre pickup on a thin, single-pack or not yet cured coating | Grind the failed patch back to concrete and lay a two-pack system |
| Cracks in the coating | The slab moved: a crack or joint below has telegraphed through | Treat the crack as live or dead, carry joints through, then repair |
| Yellow or amber tint | UV and heat on standard epoxy | Abrade and add a UV-stable topcoat |
| Slippery when wet | Smooth gloss finish with no texture | Abrade and recoat with anti-slip aggregate in the topcoat |
| Soft, tacky patches days later | Cure problem: mix ratio, mixing or cold | See our page on epoxy that is not curing |
Almost every row above goes back to the slab and the conditions on the day, not the tin. That is why the first question with any failed floor is the same: is the coating still stuck to the concrete or not? A bonded floor with surface faults can usually be keyed and recoated. A floor that is lifting cannot be saved by putting more resin on top of it.
Peeling and delamination
Delamination is the coating letting go of the concrete. You see it as flaking at the edges, patches that sound hollow when tapped, or whole sheets that peel up like a plastic skin. Resincoat puts it plainly on its help pages: a poorly prepared concrete surface is the main reason a coating peels, and the main problems are a bad surface profile and laitance.
Laitance is the weak, dusty skin that forms on top of concrete when it is laid. It looks solid, but it snaps away from the slab under load and takes the coating with it. Power-floated concrete is worse: the floating crushes the surface pores shut, so the resin sits on top with nothing to key into. Everest warn that epoxy put straight onto it can peel off in large sheets within months. Rust-Oleum's sheet for its Epoxyshield garage coating says the same about smooth, dense concrete and concrete with a curing compound on it: either one prevents a good bond.
The other usual causes of a floor lifting:
- Old paint or sealer underneath. If the coating below starts to fail, everything on top of it fails too. Resincoat do not recommend coating over an existing coat of paint at all.
- Oil, grease and dust. Flowcrete list oils, grease, chemicals and dust as things that stop resin bonding. Acid etching does not get through them: the acid just sits on the grease.
- Etching instead of grinding. Rust-Oleum's Pegakote sheet says mechanical preparation, blasting or diamond grinding, is mandatory and that chemical etching is no alternative.
- Cold or damp during the cure. Resincoat name moisture during curing as one of the biggest causes of delamination, and a cold application as a cause of flaking from low adhesion.
The trade test for a slab is how hard it is to pull off. KDR's epoxy primer sheet asks for concrete of at least 25 N/mm² compressive strength and 1.5 N/mm² pull-off strength, with the laitance and any old treatments removed. Our comparison of resin and floor paint covers why a painted garage floor peels; the cause is the same on a badly prepped resin job.
How it is fixed
Blisters from damp coming up through the slab
A blister that appears weeks or months after the floor went down, often with liquid inside, is usually osmotic blistering. Resincoat describe it as water pushed up through the slab after the coating has cured. The water cannot pass through the resin, the pressure builds, and it forms pockets of swelling. Flowcrete say high moisture coming through a slab can cause blistering and widespread delamination.
British garages are prone to it. Everest point out that many older garages, roughly pre-1980s, were built with no damp proof membrane under the slab at all. Trade epoxies ask for a slab at least 28 days old and no more than 75% relative humidity at the surface, per KDR's sheet. A quick check at home is the plastic sheet test: tape a heavy plastic sheet to the floor, leave it 24 hours, and if the concrete underneath has gone darker or there are droplets on the plastic, the slab is too damp for a standard coating.
Damp does not rule out resin. Damp-tolerant two-part epoxy primers are made to stick to wet concrete, and KDR make an epoxy damp proof membrane rated for slabs up to 95% RH. The limit is standing water under pressure, which a surface membrane is not built to hold back. Our page on putting resin over cracked or damp concrete sets out where that line sits.
Can mould grow under an epoxy floor?
The documented failure on a damp slab is blistering and lifting: water trapped under a coating it cannot get through. If you find growth or dark staining under a lifted edge, the coating has already let go there, and the moisture is what needs fixing before anything goes back down. A floor laid over a membrane suited to the slab's moisture level keeps the water out of the bond line in the first place.
Damp slab or a floor that is already lifting?
Tell us what the floor is doing and how old the concrete is. We will say what it needs before anything goes down, then quote for the job in writing.
Bubbles, pinholes and outgassing
Pinholes are tiny holes in the finished surface. Craters and bubbles are the same thing, larger. They mostly come from air: air whipped into the resin during mixing, or air in porous concrete rising up through the wet coat (outgassing). The UK sheets deal with both.
- Mix slowly. Britannia, Virtus and Flowcrete all warn against over-mixing or fast mixing because it traps air. Flowcrete specify a slow-speed drill and spinner.
- Prime porous concrete. Britannia say open, porous floors need priming, and Virtus ask for two primer coats under their self-smoothing epoxy.
- Do not leave the primer too long. Virtus say a primer left more than 48 hours must be abraded and re-primed, or the topping may pinhole.
- Spiked-roll the wet coat. On self-smoothing epoxy, a spiked roller is run over it to release trapped air, finishing before it starts to gel.
A few pinholes on a sound floor are a cosmetic repair: sand the area and recoat. A floor peppered with them usually needs a full abrade and a new topcoat. If you are doing it yourself, the priming step is the one most people skip; our step-by-step for epoxying a garage floor covers it, and self-levelling epoxy has the spiked-roller detail.
A white, greasy film: blooming and amine blush
If a newly cured floor has a white, matt, greasy or waxy look, it has bloomed. The trade also calls it amine blush. Flowcrete's sheets say high humidity early in the cure can give white, matt surfaces, and Britannia's say low temperature and high humidity make it more likely. It is a cold, damp-garage problem, which makes it a British winter problem.
The UK sheets set three rules to stop it:
- The slab and the wet floor stay at least 3°C above the dew point. Virtus hold that from before the primer goes down until at least 48 hours after.
- No laying if the air humidity is, or is going to be, over 80% (Virtus). One Sika UK sheet sets 75%.
- No gas, oil or paraffin heaters. Sika note they give off carbon dioxide and water vapour, which can spoil the finish. Electric warm air only.
A bloomed surface is cleaned off and keyed before any further coat, following the maker's sheet for that product. Leave it on and the next coat bonds to the film, not the floor. The same goes for a coat left past its recoat window: Britannia's sheet asks for an abrade before the second coat once five days have passed. There is more on putting new resin over old in recoating an epoxy floor.
What happens if epoxy gets wet before it cures?
Water and condensation on a curing floor cause the bloom above and can weaken the bond. Virtus ask for the floor to be kept from damp, condensation and water for at least 24 hours, and from water for 7 days. Flowcrete say do not cover or wash it in the first 24 hours; Britannia say avoid washing it until full cure at 7 days. Once fully cured, a resin floor shrugs off water.
A floor that is still soft or tacky days later is a different fault. That is a cure problem, covered on our page about epoxy that is not curing.
Hot tyre pickup
Hot tyre pickup is the coating lifting where the car sits: you drive off and the floor comes with the tyres. Resincoat put it down to hot tyres expanding and contracting on the floor, and point out that tyres are rubber blended with plasticisers that can leave oils on the surface. Watco explain the mechanism: new, warm and wet tyres can soften conventional paints and stick to them, forming a bond that is often stronger than the paint's bond to the concrete.
The floors that suffer are thin, single-pack paints and coatings that are not yet fully cured. Everest call parking on the floor too soon the most frequent cause. A two-pack, 100% solids epoxy on a ground slab resists it, as long as the car stays off for the full cure. Rust-Oleum give 7 days for its Epoxyshield to be ready for vehicles, and Resincoat advise letting tyres cool before parking for the first week. If a patch has already lifted, it is ground back to concrete and relaid; a fresh coat over the lifted area just lifts again.
Garage floor coming up under the car?
A lifted parking bay usually means the whole floor was a thin paint or an unground slab. Tell us the size and what is on it now, and we will price grinding it back and laying it properly.
Cracking
Cured epoxy is hard and rigid. Premium Paints put it bluntly: epoxy does not handle structural movement well, and if the concrete cracks, the epoxy will almost certainly crack with it. So a crack in an epoxy floor is nearly always a crack in the slab showing through, or a joint that was coated over instead of carried through.
The fix depends on whether the crack is still moving. Altro's technical advice is that expansion joints in the slab must be carried up through the resin as a joint, live cracks can be bridged with a heavy-duty glass fibre mesh set into the primer, and dead cracks are cleaned out and filled. Where a floor sees big swings of heat, such as hot washdowns, a polyurethane system copes with the expansion better than epoxy. The full crack-by-crack method is in our page on resin over cracked concrete, and our FAQ on slab cracks has the short version.
Yellowing
Standard epoxy is not colour fast. UK makers say so on their own sheets: UV light and heat drive the change, the rate cannot be predicted, and it shows most on pale colours and blue shades. It is cosmetic and does not weaken the floor. The fix on a sound floor is to abrade it and add a UV-stable topcoat such as a polyaspartic. Which rooms are at risk and how to prevent it are on our page on whether an epoxy floor goes yellow.
Slippery when wet
A smooth gloss epoxy floor is fine dry and can be slick wet. HSE say most slips happen when a floor is contaminated with water, grease or similar, and that thicker spills need more surface roughness to keep grip. Its fine-texture example is sandpaper against plain paper. HSE rate floors with a pendulum test: a value of 0 to 24 is high slip potential, 25 to 35 moderate, and 36 or above low. In one HSE case study, textured epoxy resin flooring with high microroughness replaced a gloss floor that was very slippery when wet.
Grip is added, not inherent. We broadcast a fine aggregate into the topcoat at the grade the area needs, as set out on our anti-slip resin flooring page. An existing slippery floor that is still sound can be abraded and given a textured topcoat. Our slippery-when-wet FAQ has the quick answer.
What epoxy will not stick to
Plenty of floor problems are really a wrong-surface problem. The UK sheets name these as unsuitable or needing their own primer:
- Asphalt and tarmac (Watco).
- Stainless steel and aluminium (Watco).
- Most self-levelling compounds, levelling mortars and anhydrite floors (Watco, Rust-Oleum).
- Smooth, dense or power-floated concrete, and concrete with a curing compound, until it is ground (Rust-Oleum, Everest).
- Concrete with a water-repellent admixture (KDR).
- Elastic paint coats and any surface that moves (Rust-Oleum Pegakote).
- Damp surfaces, unless a damp-tolerant primer or membrane goes first (Watco).
- New concrete under 28 days old (KDR, Everest).
- Old paint, and old epoxy that has not been keyed. Everest compare old epoxy to glass: any spot still shiny enough to show your reflection will peel.
If you are not sure what is under your floor, our page on what resin can be laid over goes through each base.
Vinegar and acids
Vinegar is a dilute acetic acid, and epoxy does not like it. Flowcrete's chemical resistance chart rates its solvent-free epoxy coating, epoxy screed and water-based epoxy as not resistant to acetic acid even at 5%: attacked on contact or within two to three hours. That test is full immersion, which is harsher than a spill, but the message holds. Its polyurethane screed rates excellent against the same acid. A quick wipe-up is not going to ruin a floor; cleaning with vinegar week after week is a bad idea.
For everyday cleaning, stick to a pH-neutral cleaner, as set out in our resin floor cleaning and care notes. For a kitchen or food area that sees acid spills daily, the resin itself is the decision, which is why kitchen floors are specified differently to a garage.
What a failed floor looks like, and how it is fixed
A failing floor tends to show itself at the edges first: flaking along a wall or door threshold, hollow-sounding patches when you tap it with a screwdriver handle, blisters in a band where damp comes in, or the parking bay lifting while the rest holds. Worn floors look different: dull traffic lanes, scratches and chips, with the coating still firmly stuck.
The repair follows from which one you have:
- Bonded but worn, scratched or yellowed. Watco's advice is that a well-bonded coating that is not flaking or peeling can be overcoated. It is abraded until no shiny spots are left, cleaned, and a new topcoat goes on.
- Small, local damage. Resincoat suggest abrading the affected area and patching it. Expect the patch to show against older resin.
- Lifting, flaking or blistering. The bond has gone. Resincoat say remove the existing coating by grinding or sanding, taking off all loose material; Watco call for heavy abrading such as shot blasting. Then the cause, damp, laitance or old paint, is dealt with before the new floor goes down.
Why we start every floor the same way
The downsides of epoxy, laid properly
Even a perfect job has limits worth knowing before you choose it. Epoxy is rigid, so slab movement shows. Standard epoxy yellows in strong sun. It needs warmth and dry air to cure, and a week before the car goes back on. It is smooth unless grip is added, and it is not the resin for repeated acid spills. None of those is a fault in the floor; they are reasons to spec the right system. Our epoxy and polyaspartic comparison covers the faster, UV-stable option, and the garage floor resin page covers how we build a garage floor. If it is a driveway you are worried about, the disadvantages of resin driveways are a separate subject.
About this page
Who wrote this
Written by the Obsidian Resin team, who fix and lay resin floors in Great Britain, from a single garage up to a commercial unit.
Why we wrote it
People get in touch about floors that have already gone wrong, often a DIY kit or a thin paint, and want to know why and whether it can be saved. The causes and fixes here come from the UK resin makers' own data sheets and HSE guidance, so you can check your floor against them yourself.
Our honest position
We lay floors for a living, so we would rather you had one laid properly than fought a failing one. Where a bonded floor only needs a key and a topcoat, this page says so.
Frequently asked questions
- What are the most common problems with epoxy floors?
- Peeling and delamination, blisters from damp, bubbles and pinholes, a white bloom from cold humid air, hot tyre pickup, cracks from the slab, yellowing in sunlight and a slippery surface when wet. Most trace back to the slab preparation or the conditions while the floor cured.
- Why is my epoxy floor peeling?
- Usually because it never bonded to the concrete. Laitance left on, a power-floated or sealed slab, old paint underneath, oil, or damp and cold during the cure all stop the bond. The fix is to grind off the loose coating back to sound concrete and lay it again.
- What surface will epoxy not stick to?
- UK makers list asphalt, stainless steel and aluminium, most self-levelling compounds and anhydrite floors, smooth or power-floated concrete and concrete with a curing compound until it is ground, damp surfaces without a damp-tolerant primer, new concrete under 28 days old, and old paint or unkeyed glossy epoxy.
- What happens if epoxy gets wet before it cures?
- It can bloom white and lose bond. UK data sheets ask for the floor to be kept from damp and condensation for at least 24 hours and from water or washing for about 7 days. Once fully cured, water does not harm it.
- Can mould grow under an epoxy floor?
- The documented failure on a damp slab is blistering and lifting, because the water cannot pass through the coating. If you find growth under a lifted edge, the coating has already failed there and the damp has to be fixed first, usually with a damp-tolerant primer or membrane.
- Do epoxy floors crack easily?
- The resin itself is hard, but it is rigid, so if the concrete underneath cracks or moves, the epoxy usually cracks with it. Cracks are repaired and joints carried through the resin before the floor is laid.
- Does vinegar damage epoxy?
- Repeated use can. Vinegar is a dilute acetic acid, and Flowcrete rate their epoxy coatings as not resistant to acetic acid even at 5% in immersion tests. Wipe up a spill and clean with a pH-neutral cleaner instead.
- How do you fix a failed epoxy floor?
- If the coating is still bonded, abrade it until no shiny spots remain and recoat. If it is lifting, flaking or blistering, grind it off back to sound concrete, fix the cause, such as damp or laitance, and lay it again.
- What does an epoxy floor look like after years of use?
- A well-laid floor mostly shows wear: duller traffic lanes, fine scratches and the odd chip, and possibly some yellowing if it gets sun. Those are fixed with an abrade and a fresh topcoat. Peeling or blisters point to a prep or damp problem from the start.