Epoxying a garage floor yourself is a two or three day job spread over a week, and most of the work happens before a tin is opened. This is the DIY version, step by step, with the numbers taken from the data sheets of epoxy sold in Great Britain: Rust-Oleum, Watco and Polycote. If you want to see how a trade crew does the same floor with a planetary grinder and a full resin build, that is set out in how a resin floor is installed. This page is for doing it with your own hands.
The whole job at a glance
| Step | What you do | What the data sheets say |
|---|---|---|
| 1. Test the slab | Plastic sheet taped down for 24 hours; water drop test for sealer | Droplets under the sheet or darker concrete means trapped moisture (Rust-Oleum) |
| 2. Degrease | Scrub oil and grease out, rinse, let it dry | Remove oil and grease, rinse, dry completely (Rust-Oleum) |
| 3. Grind or etch | Grind or shotblast if you can; acid etch bare concrete if you cannot | Shotblasting first choice; etch "cannot be expected to achieve the same results" (Polycote) |
| 4. Repair | Fill cracks and holes with an epoxy repair product | Repair holes and cracks before coating (Rust-Oleum) |
| 5. Prime | Penetrating primer on porous concrete, power-float primer on smooth, DPM primer on damp | Overcoat EP Primer in 12 to 36 hours (Polycote) |
| 6. Mix | Whole packs, drill and paddle, 3 to 4 minutes | "Do not hand mix or divide packs" (Polycote) |
| 7. Coat | Cut in edges, roll in small sections, keep a wet edge | One coat (Rust-Oleum 5300, Watco Ultimate) or two (Watco Gloss) |
| 8. Flake or grip | Scatter chips or aggregate into the wet coat | Chips onto the wet film, section by section (Rust-Oleum) |
| 9. Cure | Walk on it next day, car back in after up to a week | 16 h light foot, 7 days vehicles at 20°C (Rust-Oleum) |
Every time on this page is at 20°C. A colder garage stretches every one of them, which is why the temperature section further down matters as much as any step.
Before you buy anything: check the slab
An epoxy coating bonds to the top few millimetres of your concrete. If that surface is damp, sealed, too young or covered in old paint, the epoxy has nothing honest to hold on to. Four checks, all free, tell you which kind of job you have.
The damp test
Rust-Oleum's EpoxyShield data sheet gives the simplest version: tape a sheet of plastic to the floor, edges sealed, and leave it for 24 hours. "If water droplets appear on the inside of the plastic or if concrete appears wet (darker in color), moisture is trapped in the concrete." Do it in a couple of spots, including the corner furthest from the door. Trade data sheets put the line at 75% relative humidity in the slab, which needs a meter to measure, but the sheet test tells you whether you have a problem worth measuring. Watco's Ultimate Garage Floor Paint is blunter: "Do not apply to damp surfaces." A damp slab is not the end of the job, it changes the primer, which is covered below.
The water drop test for sealer
Drip a little water on the floor. If it beads up instead of soaking in, the concrete has a sealer or curing compound on it, and Rust-Oleum warns that paint "may not adhere properly". Its 5300 epoxy is not recommended on smooth, dense concrete or concrete with a curing compound at all. Water that darkens the surface and soaks in is what you want to see.
How old is the concrete?
Fresh concrete is still drying out. Watco says its etch should only go on concrete "at least 4 weeks old", and the trade epoxy data sheets ask for a minimum of 28 days. A new garage base laid this month is a job for next month. Where a slab is old enough but still holding moisture, a damp-tolerant primer is the route, and Polycote sells its DPM Primer as being for "new and old concrete with residual moisture".
Old paint and power-floated concrete
Loose or flaking paint has to come off; Rust-Oleum says sand and scrape it. Its 5300 epoxy can go over "old good adhering coatings", but an acid etch cannot: Polycote's Etch IT sheet says remove "ALL old paint and loose friable material" before using it. A glassy, power-floated garage slab is the other trap. It is too smooth for an etch to open properly, which is why Polycote says shotblast it and Watco sells a separate Powerfloat Primer for it. If your slab is cracked as well, what to do with cracked concrete before resin sorts the cracks you fill from the ones you leave alone.
Prep: degrease, then grind or etch
Prep has one job: leave clean, open, solid concrete with no laitance on top. Laitance is the weak, dusty skin that forms when concrete is floated, and an epoxy bonded to it lifts with it.
Degreasing comes first
Oil drips under where the car sits are the usual culprit. Rust-Oleum's method is a scrub brush and a degreaser, a thorough rinse with fresh water, then letting the floor dry completely. Polycote treats small deposits with its Degrease IT and big contaminated areas with hot compressed air, which is a sign of how hard old oil is to shift. Do this before grinding or etching, or you spread the oil into freshly opened concrete.
Grinding or shotblasting: the manufacturers' first choice
Polycote's own etch data sheet says it plainly: "Vacuum Assisted Shotblasting is recommended as the most professional and effective preparation, and Etch IT cannot be expected to achieve the same results." The trade epoxy sheets ask for vacuum enclosed blasting or diamond grinding, followed by thorough vacuuming. For a DIYer that means hiring a floor grinder with a dust shroud and a vacuum attached. It is the only prep that also takes off old paint and opens up a power-floated slab. Go over the whole floor, edges included, and vacuum until a hand wiped across it comes up clean.
Acid etching: the fallback for bare concrete
If you cannot grind, an acid etch is what most DIY kits use. Watco Etch & Clean is hydrochloric acid based. You scrub it in with a soft broom, leave it 15 minutes "until all frothing stops" and the pink turns clear, flush with plenty of water, then let it "dry thoroughly before painting". Polycote Etch IT is brushed on, left 5 to 10 minutes and rinsed thoroughly, between 5°C and 30°C. Wear acid gloves and eye protection, and check the coating tin before you start: some ask for an etch, some do not mention one. Our page on whether epoxy is toxic covers the fumes and skin side of the whole job.
The test that tells you prep is finished
Wipe your fingers over the clean, dry floor. Rust-Oleum says that if you see dust or powder on your fingers, rinse and scrub again. Watco's version: if "a fine powdery film can still be easily removed", etch again. Polycote adds that once the floor is prepared it "must be kept clean and free of traffic", so this is the point the bikes and bins stay out.
Would rather someone else did the grinding?
Grinding is the dustiest, heaviest part of the job and the one that decides whether the coating holds. Tell us about the garage and we will quote the whole floor, prep included.
Repairing cracks and holes
Fill after the floor is ground or etched, so the filler bonds to clean concrete, and before priming. Rust-Oleum says repair holes and cracks with its EpoxyShield concrete repair products; a two-part epoxy repair mortar does the same job on bigger damage. A crack that keeps reopening is moving, and it will crack straight through the new coating. Saw-cut joints are left open or sealed with a flexible sealant, never packed solid. The full breakdown by crack type is in can you put resin over cracked concrete.
Does a garage floor need an epoxy primer?
Sometimes, and the product decides first, then the slab. Rust-Oleum's water-based EpoxyShield 5300 goes straight on clean, sound concrete with no primer step. Watco's Ultimate Garage Floor Paint says "Bare concrete, smooth or textured, should first be primed with Watco Epoxicote High Build Primer." On top of what the tin says, three kinds of slab need a primer whatever you put over them: porous and dusty concrete, glassy power-floated concrete, and damp concrete. Each takes a different primer.
Porous, dusty concrete: a penetrating epoxy primer
Polycote EP Primer is a typical one: an ultra low viscosity, two-part, 100% solids epoxy that soaks into the concrete, seals it and hardens the surface. It is rated for moisture up to 75% RH. The reason to prime here is bubbles. On porous concrete the primer is drunk in fast and leaves dry patches, and Polycote says to give those patches a second coat to cut the air released from the slab that causes "bubbles or pinholing in the top coat". Watco gives the same reason for priming textured concrete: trapped air.
Smooth power-floated concrete: a power-float primer
A slab with a polished, almost shiny finish is too tight for a coating to key into. Watco's Epoxy Gloss Coat instructions say: "If applying to hard, smooth, powerfloated concrete use Watco Powerfloat Primer." Polycote says shotblast it first, and etch only if that is not possible. On this kind of slab, grinding plus primer is the belt and braces.
Damp concrete or no membrane: a DPM primer
If the plastic sheet test fogged up, or the garage is old enough that it may never have had a damp proof membrane, a damp-tolerant primer goes on first. Polycote DPM Primer is a water-reactive epoxy made for "permanently damp concrete floors or where the DPM is not effective or missing". It has its own rules:
- The surface is "damp but not wet": no standing water.
- "A minimum of two coats", the second laid at right angles to the first, pinhole free.
- No grit or sand in the first coat: "UNDER NO CIRCUMSTANCES SHOULD AGGREGATE BE ADDED TO THE FIRST COAT", because water would bleed through it.
- Recoat after 12 hours or once it loses its tack, and over-coat within 48 hours.
- It is "not in itself a coating or floor paint" and must always have a topcoat.
A damp primer handles moisture coming up through the slab. It is not a fix for water running in. A surface membrane is not designed to resist hydrostatic water pressure, so a garage that floods or sits below ground with water pushing through needs that fixing at the structure first.
New concrete
Wait the 28 days. If the slab is past that but still testing damp, which a new base often is through a British winter, the DPM primer route above is the one the manufacturers offer. Ask the maker before coating anything younger.
Primer timing: the window has two ends
| Primer | Overcoat no sooner than | Overcoat no later than | Temperature |
|---|---|---|---|
| Polycote EP Primer (porous concrete) | 12 hours | 36 hours, or abrade it first | 10 to 25°C, above 10°C for 24 h after |
| Polycote DPM Primer (damp concrete) | 12 hours or tack free | 48 hours | 15 to 25°C ideal, never below 5°C |
The back end catches people out. Leave EP Primer longer than 36 hours and Polycote says abrade it before the next coat, or the layers will not bond to each other. Plan the primer for the evening before the day you coat. Both sheets also say keep the floor at least 3°C above the dew point until the topcoat goes on, or condensation causes "blooming" on the surface.
How much to buy for your garage
Buy on the coverage printed on your own tin, but these are the published rates worked through for an 18m² single garage and a 32m² double, inside the 15-18m² and 30-36m² sizes UK cost guides price against. Round up: porous concrete drinks more.
| Product | Published coverage | Single, 18m² | Double, 32m² |
|---|---|---|---|
| Watco Etch & Clean | 20m² per 5 L | About 4.5 L | About 8 L |
| Polycote EP Primer | 20 to 25m² per 5 kg | One 5 kg unit | Two 5 kg units |
| Polycote DPM Primer (two coats) | About 4m² per kg per coat | About 9 kg | About 16 kg |
| Rust-Oleum EpoxyShield 5300 (one coat) | About 7m² per litre | About 2.6 L | About 4.6 L |
| Watco Epoxy Gloss Coat (per coat) | 30m² per 5 L | About 3 L | About 5.3 L |
Mixing and pot life
Two-pack epoxy starts curing the moment the two parts meet, and the clock it runs on is the pot life. It differs a lot between products, so read it off your tin before you mix:
- Water-based DIY epoxy (Rust-Oleum EpoxyShield 5300): pour part A into B, stir at least 3 minutes, then let it stand before rolling, 45 minutes at 15 to 20°C, 15 minutes at 21 to 25°C. Pot life is 2 hours at 15 to 20°C, 1.5 hours at 21 to 25°C and 1 hour at 26 to 30°C.
- Solvent-free trade epoxy and primers: about 20 to 30 minutes at 20°C, with no stand time. Polycote EP Primer is about 30 minutes; trade body coats about 20 to 25.
Mix whole packs only. Polycote says "Do not hand mix or divide packs": use a slow drill with a paddle for 3 to 4 minutes and scrape the sides and bottom into the mix, because unmixed resin gives "a poor or non-cure". When you finish, do not scrape the last of the tin onto the floor, since that is where the unmixed resin sits. If a patch stays tacky for days, the cause is usually here or the temperature, and epoxy that will not cure walks through what to do. Rust-Oleum advises two people for its 1 to 2 hour window, one cutting in the edges while the other rolls. With a 25-minute trade product, two people is the only way to finish in time.
Rolling it on, and how many coats
Cut in the edges with a brush, then roll from the back wall towards the door so you never paint yourself in. Rust-Oleum says work in sections of 1.5 by 1.5 metres and keep a wet edge to stop lap marks and patchy gloss. Watco says do not over-roller: the coating darkens slightly as it cures, and working it too long leaves marks.
How many coats depends entirely on the product. Rust-Oleum's 5300 says "In general 1 coat is sufficient." Watco's Ultimate Garage Floor Paint is one coat over its primer. Watco's Epoxy Gloss Coat is two, the second "as soon as the first coat is dry (generally 4-6 hours)". Other epoxies want 16 to 36 hours between coats. Stick to your tin's window at both ends: the Polycote primer above shows that a coat left too long needs abrading before the next one will bond.
Hot tyres
Rather have a thicker floor than a DIY coat?
A roller kit lays one or two thin coats. A trade build is primer, a self-levelling or flake body and a hard topcoat. Send us the size of the garage and we will price that build in writing.
Adding flake
Flake (decorative vinyl chips) goes into the coat while it is wet. Rust-Oleum's method is to roll one 1.5 metre section, scatter chips onto it, then roll the next, overlapping onto any loose chips that landed outside the coated area. The chips "adhere permanently", hide dirt and small imperfections, and leaving them out does not change how the coating performs. Never stir them into the tin. On a trade flake floor with a clear topcoat, the excess flake is swept and vacuumed off once the base has cured, before the topcoat goes on. The full flake build is on our flake resin floor page.
Adding anti-slip
Gloss epoxy gets slippery wet, and a garage floor gets wet every time the car comes in from the rain. Two ways to add grip appear on UK data sheets. Rust-Oleum sells an antislip additive that is mixed into the epoxy. Polycote's method is to sprinkle calcined bauxite onto the wet coat, normally 4 to 8m² per kg, from 0.5 to 10m² per kg depending on how much grip you want, wearing spiked shoes, then overcoat once it has cured so the grit is locked in. Put grip where it matters most: the apron by the door and any walkway to the house. Our anti-slip resin floors show how grip is built into a trade system.
Cure times: walking, then driving
| Product (at 20°C) | Walk on it | Heavy items | Car back in |
|---|---|---|---|
| Rust-Oleum EpoxyShield 5300 (water-based DIY) | 16 hours light, 24 hours normal | 24 hours | 7 days |
| Watco Ultimate Garage Floor Paint | 8 hours light traffic | Not stated | Not stated; cure time 16 hours |
| Trade two-pack epoxy (KDR EpoCoat HB) | 12 hours | 24 hours light wheeled | 48 hours, full cure 7 days |
Every sheet adds the same warning: at lower temperatures the times go up. Treat the drive-on figure as the earliest, and in a cold garage give it longer. Full chemical resistance also takes the full cure, so mop up any oil or brake fluid that first week straight away. Once it has cured, keeping it clean is simple, and how to clean and maintain a resin floor covers what to use.
Temperature: the rule that catches British garages
Epoxy is a chemical reaction, and cold slows it to a crawl. The limits from UK data sheets:
- Rust-Oleum: air 15 to 35°C, humidity below 80%, floor at least 13°C.
- Watco Ultimate and Epoxy Gloss Coat: minimum 15°C.
- Polycote EP Primer: 10 to 25°C, and above 10°C for 24 hours after.
- Polycote: keep the floor at least 3°C above the dew point until the topcoat is on.
The line that matters most is Rust-Oleum's: "Concrete floors take a long time to warm up; make sure the previous day has also been at least 15°C prior to painting." One warm afternoon in October is not enough if the slab has been cold all week. Rust-Oleum also says mid-afternoon painting gives the best cure. In practice that makes late spring to early autumn the DIY season for an unheated garage. If you need a floor down in winter, a fast-cure system with a lower minimum is the alternative, and epoxy vs polyaspartic sets out which polyaspartics are rated for the cold.
If something goes wrong
Bubbles usually mean porous concrete that was not primed; peeling at the tyre marks usually means laitance, oil or a coating that had not cured; a bloomed surface usually means it was laid too close to the dew point. The causes and fixes for each are in epoxy floor problems, and going over an existing coat that has worn is covered in recoating an epoxy floor. If you are still choosing between a coating and a simple sealer, concrete floor sealer vs epoxy compares the two.
DIY or have it done?
Done yourself, the cost is the kit, the etch or the grinder hire, and your weekend. Done by a professional, published UK market rates put a single garage of 15-18m² at £700-£1,800 and a double of 30-36m² at £1,200-£3,000, with the mechanical prep alone at £8-£20 per m². The difference you are paying for is the grinding, the build thickness and the system: a primer, a self-levelling or flake body coat and a hard topcoat, rather than one or two rolled coats. Our garage floor cost page breaks the ranges down, and garage floor resin shows the trade systems.
About this page
Who wrote this
For anyone doing it themselves, from the Obsidian Resin team, who coat garage floors across Great Britain. Every figure here comes from the published data sheet or product page of an epoxy, primer or etch sold in Great Britain, named where it is used.
Our honest position
We lay these floors for a living, so we would like you to pick a professional job. But plenty of people epoxy their own garage and get a good floor, and the ones who do get the slab test, the prep, the primer and the temperature right. That is why those four take up most of this page.
Frequently asked questions
- Can you epoxy a garage floor yourself?
- Yes. DIY two-pack epoxy kits are made for it. Test the slab for damp, degrease, grind or etch, repair cracks, prime if the product or slab needs it, and roll it on at 15°C or above. Plan two or three working days, then up to a week before the car goes back in.
- Does a garage floor need a primer before epoxy?
- It depends on the product and the slab. Some DIY epoxies, like Rust-Oleum EpoxyShield 5300, go straight on clean concrete. Others, like Watco Ultimate Garage Floor Paint, ask for a primer on bare concrete. Porous concrete takes a penetrating epoxy primer, smooth power-floated concrete a power-float primer, and damp concrete a damp-tolerant DPM primer in at least two coats.
- Can you put epoxy on a damp garage floor?
- Not straight on. Tape a plastic sheet down for 24 hours: droplets underneath or darker concrete means moisture. A damp-tolerant DPM primer, applied in two coats to concrete that is damp but not wet, then takes the epoxy. It does not fix water pushing through under pressure.
- Should I grind or acid etch my garage floor?
- Grind or shotblast if you can. Polycote says its own acid etch cannot be expected to match vacuum shotblasting. Etching works on bare, porous concrete only: it will not remove old paint or open up a smooth power-floated slab.
- How long after new concrete can I epoxy?
- At least 28 days, the minimum on trade epoxy data sheets. Watco says its etch is for concrete at least 4 weeks old. If the slab still tests damp after that, use a damp-tolerant primer first.
- How long before I can drive on an epoxy garage floor?
- Up to 7 days for a water-based DIY epoxy such as Rust-Oleum EpoxyShield 5300, which is walkable after 16 to 24 hours. Some trade epoxies take full traffic after 48 hours. All of these are at 20°C, and a cold garage takes longer.
- How long does it take to epoxy a 2 car garage?
- Allow a day to clear, degrease and grind or etch, time for the floor to dry, a day to repair and prime, and a day for the coats, depending on the recoat times on your tins. Then the cure: up to 7 days before you park on it.
- What is the coldest you can epoxy a garage floor?
- Most UK DIY epoxies need 15°C in the air. Rust-Oleum also asks for the floor at 13°C or more and the previous day at 15°C, because concrete is slow to warm up. Keep the floor 3°C above the dew point too, or the surface can bloom.
- How many coats of epoxy does a garage floor need?
- Whatever the tin says. Rust-Oleum EpoxyShield 5300 is generally one coat, Watco Ultimate one coat over its primer, and Watco Epoxy Gloss Coat two coats 4 to 6 hours apart. A trade system is a primer, a body coat and a topcoat.
- Can you epoxy over old garage floor paint?
- Only over paint that is still firmly bonded, and only with a product that allows it, such as Rust-Oleum EpoxyShield 5300. Loose paint has to be sanded and scraped off. An acid etch cannot be used over paint at all, so a painted floor is a grinding job.
- How much does it cost to have a double garage floor epoxied?
- Published UK market rates put a professionally laid double garage of 30-36m² at £1,200-£3,000, and a single of 15-18m² at £700-£1,800. The top of the range is decorative work, a poured floor or a slab that needs heavy prep.