A resin-bound driveway looks simple: stone and resin, mixed and trowelled flat. The makers of the resin say the opposite, and they are the ones who field the calls when a drive goes cloudy or starts shedding stones. This page is the DIY version, done properly, with every number taken from the data sheets and installation notes of resin-bound systems sold in Great Britain: PermaBound, DALTEX, Addagrip, DekorGrip, SureSet and SUDwell. Where they disagree, we say so.
The whole job at a glance
| Step | What you do | What the makers say |
|---|---|---|
| 1. Check the base | Sound tarmac or concrete, no cracks, no movement, clean and dry | Block paving, setts, flags and loose granular bases are not suitable (DALTEX) |
| 2. Edge and prime | Solid edging on every open side, tape edges, prime the base | Edging in brick, stone, concrete or steel (Addagrip); base primed and dried (PermaBound) |
| 3. Check the weather | Dry, under 80% humidity, slab 3°C above dew point | No rain during or within 4 hours of finishing (PermaBound, DALTEX) |
| 4. Mix the resin | Part A 10 to 20 seconds, add Part B, 60 seconds | Slow speed, high-torque paddle (PermaBound) |
| 5. Mix with stone | Full kit, full bags, 3 to 4 minutes in a forced action mixer | Never a cement mixer; never over 4 minutes (PermaBound) |
| 6. Lay and trowel | Tip, lute to depth, trowel in as few strokes as you can | 18mm for driveways, 15mm for foot traffic only (DALTEX) |
| 7. Keep off | Cone it off | No foot traffic for 24 hours (DALTEX, GCL) |
Two things on that list catch most first-timers out. The base decides whether the drive cracks, and the weather decides whether it cures clear. Get both right and the rest is careful, repetitive work.
Can you really do it yourself?
Yes, but the people who make the resin are split on how far. SUDwell, which sells DIY kits, says it is achievable for competent DIYers and recommends a professional for larger projects. DALTEX, made by Derbyshire Specialist Aggregates, says resin-bound "should never be considered without training", and runs a free introductory online course. PermaBound states that its own guidance is not a replacement for proper training.
Read together, that gives a sensible line. A garden path, a patio or a small front area over a base that is already sound is a fair DIY job, and it teaches you the mix before the stakes get high. A full driveway is where the numbers in the next section start to bite.
What is in a kit, and how many you need
A full-size trade kit, the kind a PermaBound or DALTEX system comes in, is one resin kit (Part A and Part B, 6.5 to 7.5 kg), four 25 kg bags of clean, kiln-dried stone (1 to 3 mm or 2 to 5 mm), and a bag of fine sand or binding quartz. Small DIY kits from sellers such as SUDwell are scaled down and pre-weighed: roughly 1 m² at 15mm and 0.8 m² at 18mm. Either way, the rule is the same:
Never adjust the ratio
| Kit (7.5 kg resin) | Covers at 15mm | Covers at 18mm |
|---|---|---|
| PermaBound | Up to 4 m² | About 3.55 m² |
| DALTEX (75 kg 2-5mm, 25 kg 1-3mm, 6.25 kg sand) | Not given | About 3.55 m² |
| DALTEX 6.5 kg resin kit | Not given | About 3.13 m² |
Now do the maths for your own space. A 10 m² path at 15mm is about three kits. A typical 60 m² two-car drive at 18mm is about 17 kits. Each 7.5 kg DALTEX kit is roughly 114 kg of stone, sand and resin, so that drive is close to 1.9 tonnes of material, mixed in 17 batches that each have to be timed to the second, laid in one dry window, and blended into each other without a visible join. That is the real difference between a path and a drive.
The base: where DIY drives usually fail
Resin-bound is a thin wearing layer, 15 to 24mm thick, and DALTEX's line is that it "will only be as good as the base beneath". If the base moves, the resin cracks with it. DALTEX lists the suitable bases as tarmac, asphalt and concrete, and is blunt about the rest: block paving, setts and flags are not suitable, because every joint underneath becomes a crack on top. It also says resin-bound "cannot usually be laid on a granular sub-base". Some kit sellers say compacted hardcore will do. We would go with the resin maker.
- Existing tarmac or concrete: firm, no movement or flexing, no cracks, clean and dry. Seal porous patches first so the resin does not soak in and cure unevenly (PermaBound).
- Brand new tarmac: give it at least 7 days. New concrete: at least 28 days (DALTEX).
- Starting from soil: one published driveway build-up (DekorGrip) is 100 to 200mm of compacted Type 1, then 50mm of porous asphalt, laid to a fall of at least 1%, before any resin goes down. The government's front-garden guidance says porous asphalt should be laid by a specialist company, so a new drive from scratch is two jobs, not one.
- Cracks and joints: cracks in concrete are broken out at least 200mm wide and filled (DekorGrip). Any joints in the base have to be mirrored in the resin surface (DALTEX).
- Manhole covers: raised to sit about 10mm above the base, at least 24 hours before laying, or swapped for recess trays you can fill with resin (SureSet).
Our page on what resin can be laid over goes through every base in depth, and resin over cracked concrete covers the repair side. One more thing to check before you buy anything: resin-bound is only permeable if the base is too. In England, a new front driveway over five square metres needs a permeable surface, or water directed to a lawn or border, to avoid planning permission. Our page on planning permission for a resin driveway has the detail.
Edges: decide them before you mix
Every open side needs a solid edge for the resin to be packed against. Addagrip specifies brick, stone, concrete or steel; SUDwell's kit checklist lists blocks, timber or aluminium. SureSet's guidance is that there needs to be some form of edge restraint to contain the surfacing, and without one the open edge has nothing to be packed against. Tape the tops of existing kerbs, walls and door thresholds so resin does not stain them. Our page on driveway edging compares the options.
Not sure your base will take resin?
Tell us what is down now, how old it is and whether it has cracked or sunk anywhere. We will say whether it can be overlaid or needs a new base first, and quote the whole drive in writing.
Weather: dew point and humidity, as well as rain
Moisture is the thing that ruins resin-bound, and DALTEX calls it "the number one enemy". Water reacting with uncured resin turns into foam or a milky cloud in the surface, and DALTEX is clear that clouding cannot be removed once cured. Rain is the obvious risk. Dew and humidity are the ones that catch people out on a dry-looking autumn morning.
| Check | Limit | Source |
|---|---|---|
| Rain | None during laying or within 4 hours of finishing | PermaBound, DALTEX |
| Humidity | Under 80% (DALTEX allows 30 to 85%) | PermaBound, Addagrip, DALTEX |
| Dew point | Surface at least 3°C above dew point | DALTEX, Addagrip |
| Temperature | +5°C to 30°C (Addagrip); 10°C to 30°C (DALTEX) | Data sheets |
| Below 15°C | Accelerator needed, dosed by temperature | DALTEX |
Buy a cheap outdoor hygrometer and record the air temperature, humidity and ground temperature before you start and as you go, which is what PermaBound tells its own installers to do. The accelerator dose changes with the thermometer: DALTEX gives 5.1 ml per 7.5 kg kit at 17.5°C, rising to 33.8 ml at 10°C. Pre-catalysed and moisture-curing resins are different again, so follow the sheet for the resin you actually bought. Hot weather has its own problem: the mix sets faster, faster still on black tarmac, so start early, keep the stone and resin in shade, and cover them with reflective blankets.
UV-stable resin, or a drive that darkens
There are two families of resin. UV-stable (aliphatic) resin holds its colour. Non-UV (aromatic) resin is slightly cheaper, and DALTEX says it can darken in sunlight in as little as two weeks. Worse, anything that sits on the drive, a car, a bin, a plant pot, keeps the original colour underneath while the rest goes darker, so you get a lighter shadow of your car. For a decorative bound driveway in any colour, buy UV-stable resin and check the data sheet says so. Our page on resin driveway colours and styles covers choosing the stone.
Mixing: a forced action mixer and a stopwatch
DALTEX traces loose stones on a finished drive to "poorly mixed aggregates where insufficient resin has coated the stone", and says cement mixers are not suitable for resin-bound. A forced action pan mixer is what the makers specify. PermaBound puts it simply: "Always use a forced action mixer. Never use a cement mixer." The small DIY kits are the one exception: SUDwell mixes those in a tub with a powerful drill and mortar paddle, and warns that a small household drill may burn out.
- Stir Part A on its own for 10 to 20 seconds at slow speed, add Part B, mix about 60 seconds until even.
- Put all four bags of dry stone in the mixer, add the mixed resin and start a stopwatch.
- Add the sand or binding quartz and mix 3 to 4 minutes in total. Never over 4.
- Tip into a lined wheelbarrow straight away and clean the mixer before the next batch.
- Time every mix the same. DALTEX traces stripy, patchy drives to batches mixed for different lengths of time.
- Keep the stone bone dry and in shade. Damp stone is moisture in the mix.
Once mixed, the clock is running. SUDwell's resin starts to cure in about 10 to 15 minutes, and PermaBound's resin gives about an hour at 21°C. That is why the makers all recommend three people: a mixer, a luter who barrows and spreads, and a troweller who finishes.
Laying and trowelling
Trowelling is where a DIY drive shows. Too many passes drag the stones and leave a scuffed, uneven surface; too few leave it open and loose. The makers' guidance is consistent:
- Mark the area in squares with chalk or marking spray, so each batch has a target.
- Tip a manageable amount, lute or rake it to depth: 18mm for a driveway, 15mm only for foot traffic.
- Clean the trowel with white spirit before you start and about every six strokes. A sticky trowel pulls stones out.
- Work from the furthest edge inward and pack the mix hard into every edge.
- Trowel until the stones stop moving and feel solid, in as few strokes as you can.
- Leave the open edge of each section rough so the next batch knits into it.
- Scatter crushed glass or fine grit lightly over the top if you want extra grip on a slope.
- Look across the surface from low angles as you go. Marks are easy to fix wet and impossible once cured.
Rather not mix 17 batches against the clock?
Send us the rough size of the drive and what it is laid on. We will price the base work and the resin-bound surface as one fixed figure in writing.
Curing: when you can walk and drive on it
The makers give different times, mostly because their resins differ. Cone the area off and keep pets off it either way. A footprint in uncured resin has to be chiselled out and relaid with fresh mix.
| Maker | Walk on it | Drive on it |
|---|---|---|
| DALTEX | Not for at least 24 hours | Not given separately |
| GCL (PermaBound) | Nobody on it for at least 24 hours | At least 24 hours |
| SureSet | About 6 hours | 24 hours |
| SUDwell DIY kits | 12 to 16 hours (light foot traffic) | 48 to 72 hours |
| Addagrip | Varies with accelerator | Full chemical cure 7 days |
Once it has cured, check it drains. The government's guidance on front gardens suggests running a hose on it for a minute or two: there should be no puddles and the water should not run more than 200 to 300mm across the surface. Day-to-day care is a brush and a low-pressure rinse; PermaBound sets 150 bar as the limit with the nozzle 200mm away. Our page on cleaning a resin driveway covers moss and stains.
Where DIY resin goes wrong, and what causes it
| What you see | Usual cause | Avoid it by |
|---|---|---|
| Milky or cloudy patches | Rain, dew or damp stone before the resin cured | Checking dew point and humidity; covering stone; no rain for 4 hours |
| Stripes or patchy colour | Batches mixed for different times | A stopwatch and identical mixes |
| Loose stones | Cement mixer, short mix or too little resin | Forced action mixer, full kits, 3 to 4 minutes |
| Cracks | The base moving underneath | A sound bound base; carrying joints through |
| Darkening, car-shaped shadows | Non-UV aromatic resin in sunlight | UV-stable aliphatic resin |
| Scuffed, uneven finish | Too many trowel passes or a dirty trowel | Few strokes; white spirit every six strokes |
| Visible joins | Sections left to set before the next batch | Rough open edges; three people keeping pace |
| Crumbling at the sides | No edge restraint | A solid edge on every open side |
Most of these cannot be fixed by going over the top. Clouding is permanent, and a patch on a resin drive rarely matches perfectly, as our page on resin driveway repairs explains. That is why the time to be honest about the job is before the first batch.
When to hand it over
DIY makes sense for a path, a patio or a small area over a base that is already sound, with three willing people and a settled forecast. Hand it over when any of these is true:
- The base is block paving, gravel, hardcore or cracked concrete, or there is no base at all.
- It is a whole drive, where the batch count and the tonnage turn a weekend into a production line.
- You cannot be sure of a dry, mild window with humidity under 80% and no rain for 4 hours after finishing.
- The drive slopes towards the house, or water has nowhere to go.
- You want a light colour on a sunny frontage and need the resin and stone matched properly.
For a sense of the other side of the decision, UK cost guides put a laid resin-bound drive at £40-£70 per m² over a sound base, with a new sub-base adding £25-£45 per m². Our resin driveway cost page breaks that down, and resin-bound driveways is how we lay them. If you are still choosing a surface, compare resin against gravel or look at the cheapest driveway options.
About this page
Who wrote this
This one is for the DIYer, written by the Obsidian Resin team. Resin-bound surfaces are a big part of what we lay, all over Great Britain. Every figure on this page comes from the data sheet, installation notes or technical notes of a resin-bound system sold in Great Britain, named where it is used, or from the government's guidance on paving front gardens.
Our honest position
We lay these for a living, so we would like you to choose a professional job, and that is our commercial interest in plain view. A small path is a fair way to learn the material, and the people who get a good result are the ones who respect the base, the weather and the stopwatch. That is why those three take up most of this page.
Frequently asked questions
- Can I resin my driveway myself?
- Yes, but it is a big job. A path or small patio over sound tarmac or concrete is a fair DIY project. A typical 60 square metre drive at 18mm is about 17 full kits and nearly two tonnes of material, mixed in a forced action mixer, timed identically and laid by three people in one dry window.
- Can I use a cement mixer for resin bound?
- No. The makers are unanimous: always use a forced action mixer, never a cement mixer. A cement mixer leaves some stones uncoated, which shows up later as loose stones. Small DIY kits of around 1 square metre are mixed in a tub with a powerful drill and paddle instead.
- How much does one resin bound kit cover?
- A full 7.5 kg kit with 100 kg of stone covers up to about 4 square metres at 15mm or about 3.55 square metres at 18mm. Small DIY kits cover roughly 1 square metre at 15mm. Use 18mm for anything a car drives on.
- How long before I can drive on a resin driveway?
- It depends on the resin. Makers give from 24 hours up to 48 to 72 hours for vehicles, with a full chemical cure at about 7 days. Keep everyone off it for at least the first 24 hours.
- Can I lay resin bound over gravel or block paving?
- No. Resin bound needs a bound, stable base such as tarmac, asphalt or concrete. Block paving, setts and flags are not suitable because their joints crack through, and resin bound cannot usually be laid on a loose or granular base.
- What happens if it rains on a new resin driveway?
- Water reacting with uncured resin causes foaming or a milky cloudiness that cannot be removed once cured. The makers say no rain during laying or within 4 hours of finishing, and the surface should be at least 3 degrees above the dew point.
- Where can I buy a DIY resin bound kit?
- From the companies that make resin bound systems and the specialist suppliers that sell them. Kits come pre-weighed, from small 1 square metre tubs to full kits with four 25 kg bags of stone. Check the resin is UV stable before you buy.
- Can I DIY an epoxy resin garage floor instead?
- Yes, that is a different product and a different job. Our page on how to epoxy a garage floor walks through it step by step.
For the garage floor version, see how to epoxy a garage floor.