You rolled the epoxy on, waited the time on the tin, and it still grabs your sock. Or worse, the middle of the garage feels hard and the edges are gummy. Before you add another coat or reach for a heater, work out which cause you are dealing with, because the fix for one makes another worse. Everything below comes from UK manufacturers' own data sheets and help pages, in °C, for floor coatings first and casting resin after.
Find your cause: what the tackiness is telling you
| What you see | Most likely cause | Will it cure if you wait? |
|---|---|---|
| The whole floor is soft or tacky, evenly | Too cold: the slab, not the air | Usually, once the floor is warmed into the product range |
| Patches or veins softer than the rest | Under-mixing: unmixed resin left in the tin | No. Unmixed resin does not cure |
| Soft strip along the walls and edges | Cutting-in brush loaded from the tin sides | No. Same cause as under-mixing |
| The last bit of the floor is soft | Scrapings from the tin wall went down unmixed | No |
| The whole batch never firmed up at all | Wrong ratio, or a pack split and measured by eye | No |
| White, waxy or greasy film on top | Amine bloom from moisture, condensation or a gas heater | The film sits on the surface. It needs a light sand and a recoat |
| Water streaks, patchy gloss, soft areas | Water or condensation during the cure | No. Scrape out what has not cured |
| Dry to touch but marks easily, tyres stick | Part cure in the cold | Only if it gets warm enough. It is not finished yet |
Two quick checks narrow it down. First, put an infrared thermometer, or a cheap stick-on one, on the floor itself, not the wall. Second, look at where the soft bits are. A floor that is evenly soft points at temperature. Soft bits with a pattern (edges, one end, streaks) point at mixing. Remmers says it plainly on its epoxy data sheet: "Streaks indicate insufficient mixing."
Cause 1: the floor was too cold
Epoxy cures by a chemical reaction, and that reaction slows right down in the cold. Remmers puts it simply: "Curing is accelerated at higher temperatures and delayed at lower temperatures." In a British garage this is the number one cause of a floor that is still tacky after 24, 48 or 72 hours.
The catch is that the temperature that counts is the slab's, and concrete is the coldest thing in the room. Watco, the UK floor-paint maker, says a heater warms the air "but not the floor, which is usually around 5-8°C lower than the air temperature." So a garage that reads 15°C on the wall thermometer can have a 7 to 10°C floor.
Here is what UK data sheets ask for:
| Product type | Minimum temperature | Source note |
|---|---|---|
| DIY water-based garage epoxy (Rust-Oleum EpoxyShield) | Air 15°C, floor 13°C, and the day before at least 15°C | Paint mid-afternoon for the best cure |
| Trade solvent-free epoxy (KDR EpoCoat HB) | 15°C during application and cure; materials and slab above 10°C | Keep above 15°C for 7 days afterwards |
| Trade clear epoxy (Virtus Strongcoat) | Apply between 15 and 25°C; never below 10°C during the cure | Store the tins at 15 to 25°C for 8 hours first |
| Two-pack garage paint (Resincoat) | Will not cure if applied under 7°C | An overnight drop slows the cure |
| Cold-cure epoxy (Watco) | Down to 5°C, one product to 0°C | Sold for heavy-traffic floors; the 0°C one for loading bays and walkways |
Note the Rust-Oleum line about the day before. Concrete takes a long time to warm up, so a mild afternoon after a frosty night still leaves you with a cold slab. And note the Virtus line about the tins: resin that has sat in a cold shed starts the job cold too.
The trap: dry is not the same as cured
Water-based epoxy has an extra problem in the cold. It has to release water to cure, and Watco says "in cold conditions the water cannot evaporate, so the floor won't dry." Part-cured water-based epoxy can also bloom and turn matt in the colder areas. A heavy coat of a water-based product in a cold garage is the worst case of all.
The good news: if cold is the only problem, it usually comes good. Resincoat's own help page says cold patches "will take longer to cure than warm patches" but "the paint should continue to cure and will eventually catch up with the rest of the coating." Warm the room safely (see below), and give it time.
Cause 2: the resin and hardener were not mixed properly
This is the cause that will not fix itself. Easy Composites says it on its GlassCast data sheet in one line: "Any resin that has not been thoroughly combined with hardener will not cure." No amount of waiting or warming changes that.
UK makers name the specific ways it goes wrong:
- Mixing by hand. KDR says "Never mix by hand." Resincoat says all two-pack products "must be mixed mechanically", with a drill and paddle. A stick in a big tin can leave veins of unmixed resin.
- Not mixing long enough. KDR asks for at least 5 minutes, scraping down the sides after 2. Virtus asks for at least 3 minutes with a slow drill (200 to 500 rpm), scraping the sides and bottom several times, "as unmixed material will result in uncured patches in the final finish."
- Scraping the tin at the end. The layer stuck to the wall of the tin "probably hasn't mixed with the part B fully", Resincoat says. If you scrape it out, mix it again in the scuttle before it goes on the floor. Otherwise the last strip you roll is the soft one.
- Loading the cutting-in brush from the side of the tin. Same problem, and it is why soft edges along the skirting are so common. Load the brush from the mixed scuttle, or from the centre of the tin.
- Mixing in one container only. Remmers and Easy Composites both tell you to mix, pour into a second clean container, and mix again. That stops unmixed resin from the bottom and sides of the first pot ever reaching the floor.
A floor with this problem usually feels mostly fine, with an area that is "slightly softer or has a slightly sticky feel when the rest of the coating has fully cured," as Resincoat describes it. That pattern is the giveaway.
Cause 3: the ratio was wrong, or the pack was split
Epoxy is not like a cake mix, where a bit extra of one thing changes the taste. The resin and hardener react in a set proportion. Easy Composites: "Failure to do so will result in a poor or only partial cure of the resin. Under no circumstances add 'extra hardener' in an attempt to speed up the cure time; epoxies do not work in this way." Too little hardener and there is resin left with nothing to react with. Too much and there is hardener left over. Either way, part of what you poured stays soft.
For floor coatings the ratio is set by the tins. Trade and DIY floor kits are sold as matched packs, and the makers say to mix the whole lot. Virtus: "Both liquids are pre-weighed and designed to be mixed together in their entirety." KDR: "Do not split packs." Resincoat goes further: taking smaller amounts from each tin, "even if measured correctly, may cause issues with the activation of the curing process", and splitting voids the warranty. If you split a garage kit to do half the floor, that alone can explain a batch that never set.
If you are mixing craft or casting resin by weight, Easy Composites asks for accuracy to within 1 to 2 grams on small mixes. Digital scales beat measuring by eye every time.
Soft floor that is not getting any harder?
If the floor has been warm for days and it is still gummy, it will need scraping back and relaying. Tell us the size of the space and we will quote to strip it and lay it properly.
Cause 4: humidity, condensation and amine bloom
Water is the enemy of curing epoxy. Resincoat lists water among the chemicals that "can react with the hardener before the paint has chance to cure". Moisture during the cure shows up two ways.
A white, waxy or greasy film on top
This is amine bloom, also called amine blush or epoxy bloom. Resincoat describes it as "a white, waxy surface on top of the coating", caused mostly by moisture, humidity, condensation or dew reaching the epoxy while it cures. Gas space heaters add moisture too. Bloom does not usually affect durability, but the surface looks patchy and feels greasy. The fix is one further coat over the top, and if the floor has been down more than 48 hours, a gentle sand with fine to medium paper first so the new coat has a key.
Streaks, patchy gloss and soft spots
Direct water or condensation landing on the floor while it cures gives "an uncured or patchy floor", according to Resincoat, which also warns against air conditioning and underfloor heating during the cure. Where it has not cured, scrape it out. Where it has, sand it to a white, hazy surface, vacuum, and recoat. If the moisture is coming up through the slab because there is no working damp-proof membrane, a recoat will not hold: the coating has to come off and the damp has to be dealt with first.
Dew point: the number to check
The dew point is the temperature at which the air's moisture condenses onto a surface. UK sheets from KDR, Virtus and Remmers all ask for the slab to stay at least 3°C above it while the epoxy cures. Virtus also says not to start if humidity is, or is expected to be, over 75%. Rust-Oleum puts its DIY limit at below 80%. Remmers explains how to check: measure the air temperature and humidity with a thermohygrometer and read the dew point off a dew point table. If conditions are wrong, it says, use heating or a dehumidifier. On a cold British evening a slab can drop below the dew point fast, so check it before you mix, not after.
Protect a fresh floor from water too. KDR asks for at least 48 hours free from damp, condensation and water at 20°C. Virtus asks for 7 days before the floor meets water. That rules out mopping, and it rules out a wet car parked on it too early.
Cause 5: it went on too thick
Floor coatings have a coverage rate for a reason. Virtus tells you to apply its epoxy "taking care not to exceed the coverage rate"; it is made to go on at about 200 microns a coat. A thick puddle in a dip or at the end of a run is often the last bit to firm up, and with a water-based epoxy, a heavy coat has more water to lose in a cold room. Polyaspartic topcoats are the same: Virtus says its polyaspartic needs humidity from the air to cure, so a film beyond the recommended 250 microns "will take a significant amount of time to through cure."
Casting and deep-pour resin works the other way. Too thick a pour does not stay soft, it overheats. Easy Composites sets a maximum pour depth for GlassCast 50 of 25 mm into wood or an insulating mould at 15 to 20°C, dropping to 18 mm at 25°C, and warns that going deeper can make the resin "dangerously overheat". Thicker pieces are built up in layers.
Cause 6: old or badly stored resin
Two-pack resin has a shelf life, and it is shorter than most people expect for trade products. KDR and Virtus both give 12 months unopened; Easy Composites gives 12 months for GlassCast. The DIY Rust-Oleum kit gives 5 years. Storage matters as much as age: KDR says store at 10 to 25°C and "Do not expose to freezing conditions." A kit that has spent a winter in the garage is a suspect.
Clear casting resin stored cold can crystallise, going cloudy, flaky or even solid in the tin. Easy Composites says that is reversed by warming the sealed container to around 40 to 50°C in hot water, then letting it cool fully to room temperature before use, because using it warm can set off an exotherm.
Will tacky epoxy eventually cure?
It depends entirely on the cause, which is why the table at the top matters:
- Cold: yes, usually, once the slab is warmed into the product's range and kept there. Resincoat says cold patches "will eventually catch up".
- Under-mixed, wrong ratio or a split pack: no. Unreacted resin or hardener stays soft however long you wait.
- Water or condensation during the cure: the affected areas generally do not recover. Scrape them out.
- Amine bloom: it does not usually affect durability, but the patchy film stays until it is sanded and recoated.
As a yardstick, UK floor epoxies at 20°C take foot traffic in about 12 to 24 hours and reach full cure in about 7 days (KDR, Rust-Oleum, Remmers, Virtus). Casting resin is slower: GlassCast 50 is touch-dry in around 48 hours and needs 72 hours at 20°C, or 96 hours at 15°C, for its initial cure. So a garage floor still gummy after 4 days in a warm room is not slow, it has a mixing or ratio problem. The same floor at 8°C may simply not have started.
To test it, wear gloves (Easy Composites says always wear them when testing a cure) and press a fingernail in. Firm resin that takes a nail mark but leaves nothing on the glove is part cured and firming. Anything that transfers to the glove is still wet.
How to fix it: remove and redo, or recoat over?
When you can wait
If the floor is evenly soft and the slab has been cold, warm the space safely and give it time. Resincoat's first fix "may be as simple as waiting for the temperature to increase a little".
When it has to come off
If it is still soft once warm, or the pattern says mixing, the makers' fix is removal, not a coat on top. Resincoat's steps:
- Scrape and abrade off as much of the soft or uncured material as you can, and wipe away the residue with a suitable solvent.
- Let the area dry fully.
- Sand or abrade the whole area so it has a good key.
- Apply a complete new coat, mixed and laid exactly to the instructions.
Putting a fresh coat straight over gummy epoxy is laying a hard skin on a soft base. It has nothing firm to bond to. Get the soft material off first. If the fault is rising damp, the whole system comes off and the damp gets fixed before anything else goes down. For the wider list of what goes wrong with these floors, see our page on common epoxy floor problems.
When a recoat is the right fix
Recoating over the top is the right call for a cured floor with a cosmetic fault: amine bloom, or patchy gloss where the coat underneath is hard. Sand the surface to a key if it has been down more than 48 hours, vacuum, and lay one more coat. Mind the overcoat window: Virtus says that once 36 hours have passed, the first coat should be abraded before the next goes on. Our page on recoating an epoxy floor goes through the prep step by step.
Would rather not strip it yourself?
Scraping back soft epoxy and keying the slab is a slow, messy job. Tell us what went down and when, and we will quote to grind it back and lay a new floor.
How to speed up epoxy curing safely
Heat is what speeds up epoxy. The question is how you add it, because the wrong heater causes the problems on this page.
- Use electric or indirect warm air heat. KDR says "do not use paraffin, oil, gas of fossil fuel heaters as they produce water vapour and carbon dioxide which adversely affects the floor finish." That water vapour is what causes amine bloom. Resincoat also says no open-flame heaters, and none that produce condensation.
- Warm the slab before you start, as well as the room after. The floor runs 5 to 8°C below the air. Heat the space the day before and keep it warm through the cure: KDR asks for 15°C for 7 days.
- Bring the tins in. Store the kit at 15 to 25°C for at least 8 hours before mixing, as Virtus asks.
- Watch the dew point. If the air is damp, a dehumidifier helps alongside the heat. Remmers names both.
- Never add extra hardener. It does not speed epoxy up; it leaves part of it uncured.
- Use a faster product next time. For a cold garage, a cold-cure epoxy rated to 5°C, or a polyaspartic, is the real fix. Our comparison of epoxy and polyaspartic covers which cures where, and our fast-cure polyaspartic floors are laid for exactly this problem.
For casting resin the rules are tighter, because extra heat can tip a deep pour into an exotherm. Easy Composites warns against radiators, direct sun and heavy heat-gun use near curing resin. Its optional post cure for GlassCast, 24 hours at room temperature then 16 hours at 60°C, is a controlled procedure for finished castings, not something to do to a garage floor with a heat gun.
Getting it right first time
Nearly every soft floor traces back to the same handful of things, so the checklist is short. Warm the slab, and check it with a thermometer on the floor. Check the dew point. Bring the tins up to room temperature. Mix whole packs with a drill and paddle for the full time, scraping the sides, then pour into a second container and mix again. Never scrape the tin onto the floor unmixed, or load your brush off its wall. Lay it at the coverage rate. Keep water, mops and gas heaters away for the cure time. And prep the slab properly: our page on how a resin floor is installed covers the grinding and moisture checks, and how to epoxy a garage floor walks through the DIY job from start to finish. If you are weighing up DIY paint against a laid floor, our resin floor versus floor paint comparison and the garage floor resin page set out the difference.
About this page
Who wrote this
Obsidian Resin put this page together. Our crews mix and lay epoxy for a living, on floors all over Great Britain.
Where the figures come from
Every temperature, time and instruction here is from UK manufacturers' published data sheets and help pages: KDR Resin Systems, Virtus Resins, Remmers UK, Rust-Oleum's UK EpoxyShield sheet, Watco, Resincoat and Easy Composites. Products differ, so the sheet for the product you used is the final word on its own temperatures and times.
Our honest position
We would rather lay your floor than see you redo one, and that is our commercial interest in plain view. But most of the fixes on this page are DIY jobs, and if your floor only needs warming up, warm it up.
Frequently asked questions
- Why is my epoxy floor still tacky after 24 hours?
- Usually because the slab is too cold. Floors run about 5 to 8°C colder than the air, and most floor epoxies want the slab at 10 to 15°C or more. If the whole floor is evenly tacky, warm the space with an electric heater and give it time. If only patches or edges are tacky, the resin was not mixed fully, and those areas will not cure on their own.
- Why is my epoxy still tacky after 48 or 72 hours?
- At 20°C, UK floor epoxies take foot traffic in about 12 to 24 hours, so a floor still tacky at 48 to 72 hours is either very cold or badly mixed. Check the floor temperature first. If it has been warm and the floor is still soft, the cause is mixing or ratio, and the soft material needs scraping off and recoating.
- Why is my epoxy still tacky after 4 days?
- If the room has been warm, four days of tackiness points to under-mixing, a wrong ratio or a split pack. That resin will not cure. If the slab has been cold the whole time, it may simply not have got going, and Resincoat says cold patches should catch up once warmed.
- Will tacky epoxy eventually dry?
- Only if the cause was cold. Warm it into the product range and it usually catches up. Resin that was never properly mixed with its hardener, or mixed in the wrong ratio, stays soft for good. A floor that loses its tack in the cold can also look dry without being fully cured, so give it its full cure time once warm.
- How do I fix epoxy that will not harden?
- Warm it first if the floor has been cold. If it is still soft once warm, scrape and abrade off as much of the soft material as you can, wipe the residue with a suitable solvent, let it dry, sand the whole area for a key, and lay a complete new coat mixed exactly to the instructions. Do not lay a fresh coat over soft epoxy.
- What happens if you mix too much hardener with resin?
- Part of the mix never reacts, so you get a poor or partial cure, the same as too little hardener. Easy Composites says never add extra hardener to speed up a cure, because epoxies do not work that way. With floor kits, mix the whole of both tins together; the makers pre-weigh them for that.
- What does tacky resin look like?
- Often it looks fine. It can be glossy and even, and only the touch gives it away: it grabs a gloved finger or takes a print. Under-mixed areas may show streaks or veins. A white, waxy or greasy film is amine bloom from moisture. A floor laid in the cold can lose its tack and look dry while still being only part cured.
- How can I speed up epoxy curing?
- Raise the temperature of the slab and the room with an electric or indirect warm-air heater, starting the day before. Never use gas, paraffin or other fuel heaters: they put water vapour into the air and cause bloom. Keep the air above the dew point, use a dehumidifier if it is damp, and never add extra hardener.
- How long does garage floor epoxy take to cure?
- At 20°C, UK data sheets give about 12 to 24 hours before you can walk on it, and about 7 days to full cure. One trade epoxy (KDR) takes full traffic after 48 hours; the DIY Rust-Oleum kit says 7 days for vehicles. Every one of those times gets longer in a cold garage.
- How long until resin becomes tacky?
- Once mixed, floor epoxy gives you a working time of roughly 15 to 25 minutes for trade products, or 1 to 2 hours for DIY water-based kits, before it starts to set. It then firms through a tacky stage over the following hours. Clear casting resin is slower: GlassCast 50 takes around 48 hours to become touch-dry.
- Can I put a new coat over tacky epoxy?
- Not over soft, uncured epoxy: the new coat has nothing firm to bond to. Scrape the soft material off and key the floor first. A recoat is right over a cured floor with a surface fault such as amine bloom, with a light sand first if it has been down more than 48 hours.